Some standard content:
IC5 59. 080. 30
Textile Industry Standard of the People's Republic of China
FZ/T73021--2004
Knitted school uniform
Issued on 2004-07-03
National Development and Reform Commission of the People's Republic of China Implemented on 2004-11-01
F7./T73021-2004
According to the American Society for Testing and Materials standard ASTM[>21G62001 Standard Performance Specification for Knitted Sportswear for Adults and Children 3, this standard is not equivalent to ASTMT)11562UU1 standard. This standard is issued by the China Textile Industry Association. This standard is jointly issued by the National Medical Products Standardization Technical Committee and the National Knitting and Environmental Standards Committee: National Knitting Product Quality Testing Center, Shenzhen Metrology Quality Inspection Research Institute, Beijing Garment Quality Supervision and Inspection Bureau, Shenzhen Liantou Garment Co., Ltd. The main drafters are Liu Fenglai and Xin Zhi. This standard is released for non-peak and seasonal changes.
1 Scope
Knitted student uniforms
FZ/73021—2004
This standard specifies the size, requirements, test methods, period, product instructions, packaging, transportation and storage of soft knitted student uniforms. This standard is only for knitted student uniforms with knitted fabrics as the main product. 2 Normative references The following documents shall apply to the provisions of this standard. The following documents shall apply to all subsequent revisions (excluding errors or revisions) of this standard. However, the parties to the revision of this standard are encouraged to study whether new versions of these documents can be produced. For any document that is not subject to review, the latest version shall apply to this standard. (50199, 1105422:199321 Certification Station Color (GB2511990105A393) GR/1353.1-1335.3 Equipment Type Number GB: 291 Product - Component Comparative Analysis Method for Product Quality Comparison GBT2910:1S97.q1S) 533:IS77 GB/T 2911
All products group three red vitamin energy system product quantitative comparison method (G3/T2911-[S7.eS508315:6)
Milk products Part 1: Hydrolyzed methyl methacrylate (water extraction method product color fastness G-
Textile color half-life test washing color oil content: test (GB/3921.11997, V1S0105GB:T321.1
Co-:1389)
GB:T 3522
Building product full car virtual test method (B332-15951S105-E0414) G/T4A5T Knitted fabrics clothing
GB/T 4892.-1
Weak-contract fabrics health test
5. Instructions for use of consumer products Textiles and clothing instructions for use Textile regulations
B/7513 Determination of H content of shrinkage products B/7—2002.IS037198UM0GT/TR529 Washing and dyeing procedures for shrinkage products (Gn/T4G2D—G.1.e9VIST)6AA5:2000) Cotton needle underwear
GHTSIS
GH/T 143T
F2/T3:031
FZ/TIU53
Textiles test method for color fastness to light and sweat 1993 knitted hook and elastic woven fabrics light elasticity and elongation rate of small and stretch textiles and the identification of the industry
F7/T01C57.:~01057.11 nano-woven wheel will be the test piece method FZ/T1055 product atmosphere to give the product drug content test characteristics GS161523-02 needle movement start photo
3 type
lunch weaving student release type this setting recovery G13T:335.1-133 yuan.? Or line 13 door 641 provisions to choose or line, 4 requirements
to The products are divided into two categories: internal quality, external quality, and external quality: internal quality, including the rate of pre-heating, the rate of twisting after water selection, the rate of color development, the degree of friction fastness, the light perspiration recovery, the pilling, the daily formaldehyde content, the visible light energy point, the size of the product, etc. 4.1.2 The quality grades of textile products are divided into two categories: internal quality, including the rate of evaluation of internal quality, and the rate of evaluation of appearance quality, and the lower one is the higher grade. 4.2 Internal quality requirements
4.2.1 Internal air volume requirements Table 1.
Table 1 Internal quality requirements
General quality
Tolerance;
Water level
Water extraction: (%)
1/12 standard area
Pure household technology/grade
(dark color)
1:12 standard dark
Darkness (lake color)
Front light. Note: Tairen sits on the monitoring grade
Super efficiency·grade
(gkg)
Fiber content
·quality
2. 2 +2.u
5 5~ -2. 3
directly accept the skin reading 76, directly accept the reflection n0 or financial skin 4.1--7.5,
non-accounting technology memory easy skin 1.U~0.
number FZ:T5:specified heat,
4.2.2 internal quality disk service items book actual inspection tools for the evaluation of this batch of products according to the trend 4.2! When the red standard is marked in the standard, the actual content of clothing is less than the actual car special standard.
4.4 to, the sample level is not strictly tested for pilling. 4.2.5 The shrimp is not specially performed under the small change rate of the size: the size change rate of the washing is not known. 4.3 Appearance quality requirements
4.3.1 Appearance quality personnel detailed year model table internal statistics point size [will be the difference car size difference, the line specified by the calculation to determine. In the same product! There are appearances that cannot be matched, and the lowest quality low point certificate can be obtained. 4.3.2 Table and symptoms evaluation and other regulations
Surface energy evaluation and other regulations see Table 2
Flow point
Color:)
Red discount is not big
Information, Erde line
Too teaching flower learning
Silk protection tight · Jia purple silk)
Anti-Yu Pingfu
Table 2 Surface symptoms evaluation and other regulations
Note the product
Main material: Selection, main property 3 one,
Contact us 2 with
F2/T73021—2004
Capital, the deposit department is not allowed, the head other parts have been obtained as the ten categories of department representatives: This introduction record
Secondary belt should: Korean effect general allow
Not allowed
Secretion limit time minister point greater than:. 3 cl
light belt design
cannot afford to over
surface age no service if 1cm one place
secretion interval extension not more than 0. 5 cm
mutual not too? m
gold car small
deep space chain flat take low when
note: not marked inside the clothing on the point: H1Xxx hit the ten points to the surface and other designated collection line note 2: Yan Shang wholesale point type clothing order underwear agricultural internal flow point color he mixed according to the effect of the limit position difference 0.3em package
gold called parts etc. 1: order deduction rate is not allowed
note: the main part of the school on the post structure, one part of the high business book theory no upper part 4.3.2.2 in the same piece of product main with no net period of the same taste no limit surface symptoms, the trend of transport promise downgrade one level. 4.3.3 see the next difference 3.
Table 3 Specification size deviation
4.3.4 Ten * Table 4.
Free products
em above
Unit medical skills
FZ/Door 73021—2004
Door dream, left enough reputation
front, back study
Chest (warmth) width is not
left and right lines
long and smooth.
Attached…
Back size is different
Table 4 Body size is different
160m and below
Excellent product
4.3.5 Garment measurement and determination (accurate to (1crs) 4.3.5.1 Long shadow mark most part see =
4.3.5.2 Middle draw shirt measurement part model 2
4.3.5.3 Stall horizontal measurement part see Figure 3.4.3.5.4. The measurement part should be medical 1.
Yifang filling
-quality
Figure · Long grapefruit color creation measurement part
Superior product
1tm or more
Single busy is a meter
2-pulse gram
Single gram:
Sample length:
2-vertical;
Tops
Ready-made clothing measurement part regulations
Determined width
National 2 half-sleeve measurement position
National 3 trousers orange most part
Figure 4 row of vertical measurement period
Table 5 Production measurement part regulations||tt ||Production quantity at the bottom
Extraction key solution contains the following 2 quantities: including the moving area according to FZ/T73021--2004
to the edge from the back time
out of the left and note the production must point white year to the direction and into the negative intersection of the body and clothing inspection by the automatic monitoring risk determination distance sense Fz/T73321—2004
4.3.6 allowed when the current determination
4. 3. 6.2
Table 5 continued?
The world's teeth are folded in order to achieve the same needle quantity. The relative position of the reverse body: please check the angle of the equivalent quantityWww.bzxZ.net
The order of the joint should be added with the original material dot pattern strip or banknote tape, and the joint should be sewn on the bag machine. The joint trace is read with F1 thread and the upper end of the bag is sewn for the second warp. The speed of the flat sewing machine is adjusted to create the second mouth. The dynamic bag can be stitched and added along the static joint.
4. 3. 6. 7
No machine model maintenance: For those who use the bag to sew, the back collar part uses a double-lead machine to thank the color collar strip. The collar type is down, the momentum is a hundred, and the words can be pulled off. The line is repaired and cleaned by the three-blood single oxygen phase method. The original large residual begins. The selection is not deformed, rusty, or discolored. The speed is required.
Table E Stitch Density Provisions
4. 3. 6, 9
What is the shortage of machine
fine sleep machine
Measure the stitch density with a chain stroke in the middle of the process without any gap
Single number: 2m
Reverse machine
4.3.6.10 Limit machine density, 4 is used to measure 2-3 stitches at both ends, 4. 3. 6. 11
4. 3.6. 12
The needle penetration rate of the scan shall not be less than 5 stitches. Continuous plate chain problem: 3.m:
present hoop machine
4.3.6.13 Chain needle change setting shall not be less than 5 yuan. Each part of the seam shall not have two continuous auxiliary stitches within 201m. No skipping stitch is allowed.
4.3.6.14 Each part of the connecting thread is broken, complete, half-row, and solid. 4.3.6.15 Each part of the sewing garment can be tested at the end of the work, 5 points, and 5.1 Sampling quantity
5.1, 1 external quality shall be collected at random. 5.1.2 The internal quality inspection machine shall collect 5 pieces. More than 5 pieces are added. 5.2 Appearance quality inspection and testing shall be carried out in accordance with the provisions of this clause (F%7H). 5.3 Sample accuracy and test items shall be tested for the breakage of marbles, joint strength, water length, and core iron sheet torsion rate. The test items shall be placed in the laboratory at a relative limit of 2%-2% under the temperature control of 533°C before the test is carried out. 5.4 Test items 5.4.1 Marble magnetic strength test shall be carried out in accordance with the current regulations. 5.4.2 Joint strength test 5.4.2. According to Fz123 regulations, the sample parts of the finished product shall be carried out in accordance with F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Test for dimensional change rate after washing. E/T73021-204
5.4.3.2 Test for dimensional change rate after washing: For tops, take the length and width of the garment as the vertical and horizontal measurement parts, and the average value of the length of the garment from front to back and left to right is used as the calculation basis. Take the side length and the middle length as the measurement parts, and then take the average value of the length in the system and the calculation basis, and take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing.
Measure the length of the garment, and then take the average value of the length in the system and the calculation basis, and then take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing. 3. Measure the reverse side and calculate the compensation point of the damage to the EM point and the compensation point of the repair. 5.4.3.4 Measure the single part of the garment before and after washing. 5.4.3.5 Measure the part of the garment before and after washing. See Figure f. Measure the part of the garment before and after washing. 5.4.4 Test for distortion rate after washing. 5.4.4.1 Test for curvature after washing. Place the finished garment on a smooth surface. Flatten it with your hand. Measure the side with the largest inclination of each garment. Take the average torsion rate of the three garments as the calculation result. 5.4.4.2 Test for the curvature of the garment after washing. 5. 1.4.2.! Philosophy agent see Figure 7.
5.4.2.2.2 Pants near the state part of the south 2.
FZ/T73021-20C4
The intersection of the border and the water protection and the intersection of the formula are higher, the health requirements,
The intersection of the upper and lower parts
The ratio of the intersection of the whole mouth and the inner effect after washing; the inner part,
The twisted part of the pants
5.4,4.3 The original formula of the mountain design sees the formula (1 The final result is accurate): F
5.4.5 Washing color fastness test
Investment R311 standard heat conduction
5.1.6 Sweat fastness test
Guest GH1 plan 22 is now implemented.
5.4.7 Color fastness to rubbing
According to (3/T3320. 5.4.8 Color fastness to light and perspiration
According to GHT157S+B.
5.4.9 Test for rubbing resistance
According to GR/T1802.1, H is 160N, rubbing times, 500 times per meter, according to G816132-2002.
5.4.10 Test for methyl ester content
According to (/,: Regulations. Special treatment products such as printing and other special treatments are tested at different places such as the rate of flower inhibition. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative design implementation,
Yifang Chong
-Quality products
Figure·Long grapefruit color measurement parts
Superior products
1tm and above
Single busy is a meter
2-pulse
Single Fu weight:
Sample length:
2-vertical;
Tops
Regulations on measurement parts of ready-made clothes
Special width
National 2 half-sleeve measurement position
National 3 trousers vertical position
Figure 4 Vertical measurement position of pants
Table 5 Regulations on measurement parts of ready-made clothes||tt ||Production quantity at the bottom
Extraction key solution contains the following 2 quantities: including the moving area according to FZ/T73021--2004
to the edge from the back time
out of the left and note the production must point white year to the direction and into the negative intersection of the body and clothing inspection by the automatic monitoring risk determination distance sense Fz/T73321—2004
4.3.6 allowed when the current determination
4. 3. 6.2
Table 5 continued?
The world's teeth are folded in order to achieve the same needle quantity. The relative position of the reverse body: please check the angle of the equivalent quantity
The order of the joint should be added with the original material dot pattern strip or banknote tape, and the joint should be sewn on the bag machine. The joint trace is read with F1 thread and the upper end of the bag is sewn for the second warp. The speed of the flat sewing machine is adjusted to create the second mouth. The dynamic bag can be stitched and added along the static joint.
4. 3. 6. 7
No machine model maintenance: For those who use the bag to sew, the back collar part uses a double-lead machine to thank the color collar strip. The collar type is down, the momentum is a hundred, and the words can be pulled off. The line is repaired and cleaned by the three-blood single oxygen phase method. The original large residual begins. The selection is not deformed, rusty, or discolored. The speed is required.
Table E Stitch Density Provisions
4. 3. 6, 9
What is the shortage of machine
fine sleep machine
Measure the stitch density with a chain stroke in the middle of the process without any gap
Single number: 2m
Reverse machine
4.3.6.10 Limit machine density, 4 is used to measure 2-3 stitches at both ends, 4. 3. 6. 11
4. 3.6. 12
The needle penetration rate of the scan shall not be less than 5 stitches. Continuous plate chain problem: 3.m:
present hoop machine
4.3.6.13 Chain needle change setting shall not be less than 5 yuan. Each part of the seam shall not have two continuous auxiliary stitches within 201m. No skipping stitch is allowed.
4.3.6.14 Each part of the connecting thread is broken, complete, half-row, and solid. 4.3.6.15 Each part of the sewing garment can be tested at the end of the work, 5 points, and 5.1 Sampling quantity
5.1, 1 external quality shall be collected at random. 5.1.2 The internal quality inspection machine shall collect 5 pieces. More than 5 pieces are added. 5.2 Appearance quality inspection and testing shall be carried out in accordance with the provisions of this clause (F%7H). 5.3 Sample accuracy and test items shall be tested for the breakage of marbles, joint strength, water length, and core iron sheet torsion rate. The test items shall be placed in the laboratory at a relative limit of 2%-2% under the temperature control of 533°C before the test is carried out. 5.4 Test items 5.4.1 Marble magnetic strength test shall be carried out in accordance with the current regulations. 5.4.2 Joint strength test 5.4.2. According to Fz123 regulations, the sample parts of the finished product shall be carried out in accordance with F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Test for dimensional change rate after washing. E/T73021-204
5.4.3.2 Test for dimensional change rate after washing: For tops, take the length and width of the garment as the vertical and horizontal measurement parts, and the average value of the length of the garment from front to back and left to right is used as the calculation basis. Take the side length and the middle length as the measurement parts, and then take the average value of the length in the system and the calculation basis, and take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing.
Measure the length of the garment, and then take the average value of the length in the system and the calculation basis, and then take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing. 3. Measure the reverse side and calculate the compensation point of the damage to the EM point and the compensation point of the repair. 5.4.3.4 Measure the single part of the garment before and after washing. 5.4.3.5 Measure the part of the garment before and after washing. See Figure f. Measure the part of the garment before and after washing. 5.4.4 Test for distortion rate after washing. 5.4.4.1 Test for curvature after washing. Place the finished garment on a smooth surface. Flatten it with your hand. Measure the side with the largest inclination of each garment. Take the average torsion rate of the three garments as the calculation result. 5.4.4.2 Test for the curvature of the garment after washing. 5. 1.4.2.! Philosophy agent see Figure 7.
5.4.2.2.2 Pants near the state part of the south 2.
FZ/T73021-20C4
The intersection of the border and the water protection and the intersection of the formula are higher, the health requirements,
The intersection of the upper and lower parts
The ratio of the intersection of the whole mouth and the inner effect after washing; the inner part,
The twisted part of the pants
5.4,4.3 The original formula of the mountain design sees the formula (1 The final result is accurate): F
5.4.5 Washing color fastness test
Investment R311 standard heat conduction
5.1.6 Sweat fastness test
Guest GH1 plan 22 is now implemented.
5.4.7 Color fastness to rubbing
According to (3/T3320. 5.4.8 Color fastness to light and perspiration
According to GHT157S+B.
5.4.9 Test for rubbing resistance
According to GR/T1802.1, H is 160N, rubbing times, 500 times per meter, according to G816132-2002.
5.4.10 Test for methyl ester content
According to (/,: Regulations. Special treatment products such as printing and other special treatments are tested at different places such as the rate of flower inhibition. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative design implementation,
Yifang Chong
-Quality products
Figure·Long grapefruit color measurement parts
Superior products
1tm and above
Single busy is a meter
2-pulse
Single Fu weight:
Sample length:
2-vertical;
Tops
Regulations on measurement parts of ready-made clothes
Special width
National 2 half-sleeve measurement position
National 3 trousers vertical position
Figure 4 Vertical measurement position of pants
Table 5 Regulations on measurement parts of ready-made clothes||tt ||Production quantity at the bottom
Extraction key solution contains the following 2 quantities: including the moving area according to FZ/T73021--2004
to the edge from the back time
out of the left and note the production must point white year to the direction and into the negative intersection of the body and clothing inspection by the automatic monitoring risk determination distance sense Fz/T73321—2004
4.3.6 allowed when the current determination
4. 3. 6.2
Table 5 continued?
The world's teeth are folded in order to achieve the same needle quantity. The relative position of the reverse body: please check the angle of the equivalent quantity
The order of the joint should be added with the original material dot pattern strip or banknote tape, and the joint should be sewn on the bag machine. The joint trace is read with F1 thread and the upper end of the bag is sewn for the second warp. The speed of the flat sewing machine is adjusted to create the second mouth. The dynamic bag can be stitched and added along the static joint.
4. 3. 6. 7
No machine model maintenance: For those who use the bag to sew, the back collar part uses a double-lead machine to thank the color collar strip. The collar type is down, the momentum is a hundred, and the words can be pulled off. The line is repaired and cleaned by the three-blood single oxygen phase method. The original large residual begins. The selection is not deformed, rusty, or discolored. The speed is required.
Table E Stitch Density Provisions
4. 3. 6, 9
What is the shortage of machine
fine sleep machine
Measure the stitch density with a chain stroke in the middle of the process without any gap
Single number: 2m
Reverse machine
4.3.6.10 Limit machine density, 4 is used to measure 2-3 stitches at both ends, 4. 3. 6. 11
4. 3.6. 12
The needle penetration rate of the scan shall not be less than 5 stitches. Continuous plate chain problem: 3.m:
present hoop machine
4.3.6.13 Chain needle change setting shall not be less than 5 yuan. Each part of the seam shall not have two continuous auxiliary stitches within 201m. No skipping stitch is allowed.
4.3.6.14 Each part of the connecting thread is broken, complete, half-row, and solid. 4.3.6.15 Each part of the sewing garment can be tested at the end of the work, 5 points, and 5.1 Sampling quantity
5.1, 1 external quality shall be collected at random. 5.1.2 The internal quality inspection machine shall collect 5 pieces. More than 5 pieces are added. 5.2 Appearance quality inspection and testing shall be carried out in accordance with the provisions of this clause (F%7H). 5.3 Sample accuracy and test items shall be tested for the breakage of marbles, joint strength, water length, and core iron sheet torsion rate. The test items shall be placed in the laboratory at a relative limit of 2%-2% under the temperature control of 533°C before the test is carried out. 5.4 Test items 5.4.1 Marble magnetic strength test shall be carried out in accordance with the current regulations. 5.4.2 Joint strength test 5.4.2. According to Fz123 regulations, the sample parts of the finished product shall be carried out in accordance with F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Test for dimensional change rate after washing. E/T73021-204
5.4.3.2 Test for dimensional change rate after washing: For tops, take the length and width of the garment as the vertical and horizontal measurement parts, and the average value of the length of the garment from front to back and left to right is used as the calculation basis. Take the side length and the middle length as the measurement parts, and then take the average value of the length in the system and the calculation basis, and take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing.
Measure the length of the garment, and then take the average value of the length in the system and the calculation basis, and then take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing. 3. Measure the reverse side and calculate the compensation point of the damage to the EM point and the compensation point of the repair. 5.4.3.4 Measure the single part of the garment before and after washing. 5.4.3.5 Measure the part of the garment before and after washing. See Figure f. Measure the part of the garment before and after washing. 5.4.4 Test for distortion rate after washing. 5.4.4.1 Test for curvature after washing. Place the finished garment on a smooth surface. Flatten it with your hand. Measure the side with the largest inclination of each garment. Take the average torsion rate of the three garments as the calculation result. 5.4.4.2 Test for the curvature of the garment after washing. 5. 1.4.2.! Philosophy agent see Figure 7.
5.4.2.2.2 Pants near the state part of the south 2.
FZ/T73021-20C4
The intersection of the border and the water protection and the intersection of the formula are higher, the health requirements,
The intersection of the upper and lower parts
The ratio of the intersection of the whole mouth and the inner effect after washing; the inner part,
The twisted part of the pants
5.4,4.3 The original formula of the mountain design sees the formula (1 The final result is accurate): F
5.4.5 Washing color fastness test
Investment R311 standard heat conduction
5.1.6 Sweat fastness test
Guest GH1 plan 22 is now implemented.
5.4.7 Color fastness to rubbing
According to (3/T3320. 5.4.8 Color fastness to light and perspiration
According to GHT157S+B.
5.4.9 Test for rubbing resistance
According to GR/T1802.1, H is 160N, rubbing times, 500 times per meter, according to G816132-2002.
5.4.10 Test for methyl ester content
According to (/,: Regulations. Special treatment products such as printing and other special treatments are tested at different places such as the rate of flower inhibition. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative design implementation,T4856 or co-implementation,T4856 or co-implementation,T4856 or co-implementation,T4856 or co-implementation,T4856 or co-implementation,T4856 or co-implementation,6. 7
No machine model maintenance: For those with upper collars sewn with a bag, the back collar part uses a double-lead machine chain with a color collar strip. The collar is shaped like a hundred, and the words can be pulled off. The line is repaired and cleaned by a three-blood single oxygen phase method. The original part is large and the residual is started. The core is not deformed, rusted, or discolored. The speed is specified in the table.
Table E Stitch Density Provisions
4. 3. 6, 9
What is the shortage of machine
fine sleep machine
Measure the stitch density with a chain stroke in the middle of the process without any gap
Single number: 2m
Reverse machine
4.3.6.10 Limit machine density, 4 is used to measure 2-3 stitches at both ends, 4. 3. 6. 11
4. 3.6. 12
The needle penetration rate of the scan shall not be less than 5 stitches. Continuous plate chain problem: 3.m:
present hoop machine
4.3.6.13 Chain needle change setting shall not be less than 5 yuan. Each part of the seam shall not have two continuous auxiliary stitches within 201m. No skipping stitch is allowed.
4.3.6.14 Each part of the connecting thread is broken, complete, half-row, and solid. 4.3.6.15 Each part of the sewing garment can be tested at the end of the work, 5 points, and 5.1 Sampling quantity
5.1, 1 external quality shall be collected at random. 5.1.2 The internal quality inspection machine shall collect 5 pieces. More than 5 pieces are added. 5.2 Appearance quality inspection and testing shall be carried out in accordance with the provisions of this clause (F%7H). 5.3 Sample accuracy and test items shall be tested for the breakage of marbles, joint strength, water length, and core iron sheet torsion rate. The test items shall be placed in the laboratory at a relative limit of 2%-2% under the temperature control of 533°C before the test is carried out. 5.4 Test items 5.4.1 Marble magnetic strength test shall be carried out in accordance with the current regulations. 5.4.2 Joint strength test 5.4.2. According to Fz123 regulations, the sample parts of the finished product shall be carried out in accordance with F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Test for dimensional change rate after washing. E/T73021-204
5.4.3.2 Test for dimensional change rate after washing: For tops, take the length and width of the garment as the vertical and horizontal measurement parts, and the average value of the length of the garment from front to back and left to right is used as the calculation basis. Take the side length and the middle length as the measurement parts, and then take the average value of the length in the system and the calculation basis, and take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing.
Measure the length of the garment, and then take the average value of the length in the system and the calculation basis, and then take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing. 3. Measure the reverse side and calculate the compensation point of the damage to the EM point and the compensation point of the repair. 5.4.3.4 Measure the single part of the garment before and after washing. 5.4.3.5 Measure the part of the garment before and after washing. See Figure f. Measure the part of the garment before and after washing. 5.4.4 Test for distortion rate after washing. 5.4.4.1 Test for curvature after washing. Place the finished garment on a smooth surface. Flatten it with your hand. Measure the side with the largest inclination of each garment. Take the average torsion rate of the three garments as the calculation result. 5.4.4.2 Test for the curvature of the garment after washing. 5. 1.4.2.! Philosophy agent see Figure 7.
5.4.2.2.2 Pants near the state part of the south 2.
FZ/T73021-20C4
The intersection of the border and the water protection and the intersection of the formula are higher, the health requirements,
The intersection of the upper and lower parts
The ratio of the intersection of the whole mouth and the inner effect after washing; the inner part,
The twisted part of the pants
5.4,4.3 The original formula of the mountain design sees the formula (1 The final result is accurate): F
5.4.5 Washing color fastness test
Investment R311 standard heat conduction
5.1.6 Sweat fastness test
Guest GH1 plan 22 is now implemented.
5.4.7 Color fastness to rubbing
According to (3/T3320. 5.4.8 Color fastness to light and perspiration
According to GHT157S+B.
5.4.9 Test for rubbing resistance
According to GR/T1802.1, H is 160N, rubbing times, 500 times per meter, according to G816132-2002.
5.4.10 Test for methyl ester content
According to (/,: Regulations. Special treatment products such as printing and other special treatments are tested at different places such as the rate of flower inhibition. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative design implementation,6. 7
No machine model maintenance: For those with upper collars sewn with a bag, the back collar part uses a double-lead machine chain with a color collar strip. The collar is shaped like a hundred, and the words can be pulled off. The line is repaired and cleaned by a three-blood single oxygen phase method. The original part is large and the residual is started. The core is not deformed, rusted, or discolored. The speed is specified in the table.
Table E Stitch Density Provisions
4. 3. 6, 9
What is the shortage of machine
fine sleep machine
Measure the stitch density with a chain stroke in the middle of the process without any gap
Single number: 2m
Reverse machine
4.3.6.10 Limit machine density, 4 is used to measure 2-3 stitches at both ends, 4. 3. 6. 11
4. 3.6. 12
The needle penetration rate of the scan shall not be less than 5 stitches. Continuous plate chain problem: 3.m:
present hoop machine
4.3.6.13 Chain needle change setting shall not be less than 5 yuan. Each part of the seam shall not have two continuous auxiliary stitches within 201m. No skipping stitch is allowed.
4.3.6.14 Each part of the connecting thread is broken, complete, half-row, and solid. 4.3.6.15 Each part of the sewing garment can be tested at the end of the work, 5 points, and 5.1 Sampling quantity
5.1, 1 external quality shall be collected at random. 5.1.2 The internal quality inspection machine shall collect 5 pieces. More than 5 pieces are added. 5.2 Appearance quality inspection and testing shall be carried out in accordance with the provisions of this clause (F%7H). 5.3 Sample accuracy and test items shall be tested for the breakage of marbles, joint strength, water length, and core iron sheet torsion rate. The test items shall be placed in the laboratory at a relative limit of 2%-2% under the temperature control of 533°C before the test is carried out. 5.4 Test items 5.4.1 Marble magnetic strength test shall be carried out in accordance with the current regulations. 5.4.2 Joint strength test 5.4.2. According to Fz123 regulations, the sample parts of the finished product shall be carried out in accordance with F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Test for dimensional change rate after washing. E/T73021-204
5.4.3.2 Test for dimensional change rate after washing: For tops, take the length and width of the garment as the vertical and horizontal measurement parts, and the average value of the length of the garment from front to back and left to right is used as the calculation basis. Take the side length and the middle length as the measurement parts, and then take the average value of the length in the system and the calculation basis, and take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing.
Measure the length of the garment, and then take the average value of the length in the system and the calculation basis, and then take the average value of the length in the system as the calculation basis, and make the mark during measurement, and then measure after washing:
5.4.3.3 Measurement parts for dimensional change rate after washing are shown in Table 7. The table shows the measurement parts for dimensional change rate after washing. 3. Measure the reverse side and calculate the compensation point of the damage to the EM point and the compensation point of the repair. 5.4.3.4 Measure the single part of the garment before and after washing. 5.4.3.5 Measure the part of the garment before and after washing. See Figure f. Measure the part of the garment before and after washing. 5.4.4 Test for distortion rate after washing. 5.4.4.1 Test for curvature after washing. Place the finished garment on a smooth surface. Flatten it with your hand. Measure the side with the largest inclination of each garment. Take the average torsion rate of the three garments as the calculation result. 5.4.4.2 Test for the curvature of the garment after washing. 5. 1.4.2.! Philosophy agent see Figure 7.
5.4.2.2.2 Pants near the state part of the south 2.
FZ/T73021-20C4
The intersection of the border and the water protection and the intersection of the formula are higher, the health requirements,
The intersection of the upper and lower parts
The ratio of the intersection of the whole mouth and the inner effect after washing; the inner part,
The twisted part of the pants
5.4,4.3 The original formula of the mountain design sees the formula (1 The final result is accurate): F
5.4.5 Washing color fastness test
Investment R311 standard heat conduction
5.1.6 Sweat fastness test
Guest GH1 plan 22 is now implemented.
5.4.7 Color fastness to rubbing
According to (3/T3320. 5.4.8 Color fastness to light and perspiration
According to GHT157S+B.
5.4.9 Test for rubbing resistance
According to GR/T1802.1, H is 160N, rubbing times, 500 times per meter, according to G816132-2002.
5.4.10 Test for methyl ester content
According to (/,: Regulations. Special treatment products such as printing and other special treatments are tested at different places such as the rate of flower inhibition. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative design implementation,3 Sample supervision and test items
Ball breakage, connection strength, water length, core iron sheet torsion rate test, the test objects will be placed in the laboratory under the relative limit of 2%-2% under constant temperature before the test is carried out. 5.4 Test items
5.4.1 Marble magnetic strength test
Perform as specified.
5.4.2 Wall strength test
5.4.2, according to Fz123 regulations, reach
5.4.2.2 Finished product sample parts according to F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Washing size change rate test issued by E/H78 period. EZ/T73021-204
5.4.3.2 Washing size change rate test measurement parts: the length and width of the top are taken as the vertical and horizontal measurement parts, and the length of the top is calculated based on the average value of the front, back, left and right sides of the body. Take the side length as the measurement part, and then take the average value of the length in the system and the calculation basis, that is, the average value of the middle limit is calculated. According to the standard, make the following measurements when measuring: 5.4.3.3 Water selection size change measurement position description see Table 7. Table 7 shows the measurement position description of the size change rate after washing. Measure the length of the garment, and then measure the reverse side. The change point can be adjusted to the EM position, and the change point can be adjusted to the position of the compensation point. 5.4.3.4 Measure the single position of the garment before and after washing. See Figure 5. 5.4.3.5 Measure the position of the garment before and after washing. See Figure f. 5.4.4 Distortion rate test after washing 5.4.4.1 The curvature of the shape after washing is measured by the small method, and the water method is completed. The garment with small size change rate is placed on the smooth price. Gently pat it flat with your hand, and measure the side with the largest inclination of each piece. The average torsion rate of 3 pieces is used as the calculation result: 5.4.4.2 The garment mountain part,
5.1.4.2.! See Figure 7 for the properties of the agent.
5.4.2.2.2 The pants near the state part is 2.
FZ/T73021-20C4
The intersection of the border and the water protection and treatment of the formula is higher, the healthier the request,
The upper intersection of the sweeping part
The ratio between the intersection of the strong and the dense hair point after washing and the inner bottom effect; the inner point,
Pressure 8 Pants twisted part
5.4,4.3 State mountain calculation formula (1 The final result is accurate): F
5.4.5 Washing fastness test
Apply to R311 standard
5.1.6 Perspiration fastness test
Apply to GH122. 5.4.7 Color fastness to rubbing test
Apply to (3/T3320 standard. Applicable direction: 5.4.8 Light and perspiration fastness test
Perform the test specified in GHT157S+B
5.4.9 Test according to GR/T1802.1, H is 160N, the number of times, the total number of times is 500 meters, and the test level is in accordance with G816132-2002:
5.4.10 Methyl acetate content test
Perform the provisions of (/,:). 5.4.11 pH value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11,HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate according to the external quality yellow core batch. If the rate of non-conforming products is within the range of 7 and below, the batch of products is qualified. If the rate of non-conforming products is above the range of 7, the batch of products is qualified.
6.1.2 Inner packaging mark is calculated, and no external error is allowed. 6.2 Inner quality
6.2.1 The inspection results will be taken from the adjacent test samples, and the qualified ones will be judged as qualified, and the unqualified ones will be judged as unqualified. 6.2.2 Calculate the dimensional change rate of all test samples and the result with acid. If the test results show that the batch of products are qualified, the unqualified ones will be determined as unqualified. If there is shrinkage and expansion test, the value of the calculated value (or the value selected by the test frequency) will be used as the test result. If the batch of products are qualified, the batch of products will be determined as qualified, and the unqualified ones will be determined as unqualified. 6.2.3 For formaldehyde content, for light color, for color flatness, for chromaticity, and for color flatness, the batch of products will be determined as qualified, and the unqualified ones will be determined as unqualified. : 6.2.4 The product performance of the product is not allowed to be released. 6.3 Re-inspection || tt || 6.3.1 The results of the inspection are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to the friend for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection time is the designated inspection quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations will be implemented, and the inspection will be based on it. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative implementation,3 Sample supervision and test items
Ball breakage, connection strength, water length, core iron sheet torsion rate test, the test objects will be placed in the laboratory under the relative limit of 2%-2% under constant temperature before the test is carried out. 5.4 Test items
5.4.1 Marble magnetic strength test
Perform as specified.
5.4.2 Wall strength test
5.4.2, according to Fz123 regulations, reach
5.4.2.2 Finished product sample parts according to F2/T (131293 Appendix F. 5.4.3 Washing size change rate test
5.4.3.1 Washing size change rate test issued by E/H78 period. EZ/T73021-204
5.4.3.2 Washing size change rate test measurement parts: the length and width of the top are taken as the vertical and horizontal measurement parts, and the length of the top is calculated based on the average value of the front, back, left and right sides of the body. Take the side length as the measurement part, and then take the average value of the length in the system and the calculation basis, that is, the average value of the middle limit is calculated. According to the standard, make the following measurements when measuring: 5.4.3.3 Water selection size change measurement position description see Table 7. Table 7 shows the measurement position description of the size change rate after washing. Measure the length of the garment, and then measure the reverse side. The change point can be adjusted to the EM position, and the change point can be adjusted to the position of the compensation point. 5.4.3.4 Measure the single position of the garment before and after washing. See Figure 5. 5.4.3.5 Measure the position of the garment before and after washing. See Figure f. 5.4.4 Distortion rate test after washing 5.4.4.1 The curvature of the shape after washing is measured by the small method, and the water method is completed. The garment with small size change rate is placed on the smooth price. Gently pat it flat with your hand, and measure the side with the largest inclination of each piece. The average torsion rate of 3 pieces is used as the calculation result: 5.4.4.2 The garment mountain part,
5.1.4.2.! See Figure 7 for the properties of the agent.
5.4.2.2.2 The pants near the state part is 2.
FZ/T73021-20C4
The intersection of the border and the water protection and treatment of the formula is higher, the healthier the request,
The upper intersection of the sweeping part
The ratio between the intersection of the strong and the dense hair point after washing and the inner bottom effect; the inner point,
Pressure 8 Pants twisted part
5.4,4.3 State mountain calculation formula (1 The final result is accurate): F
5.4.5 Washing fastness test
Apply to R311 standard
5.1.6 Perspiration fastness test
Apply to GH122. 5.4.7 Color fastness to rubbing test
Apply to (3/T3320 standard. Applicable direction: 5.4.8 Light and perspiration fastness test
Perform the test specified in GHT157S+B
5.4.9 Test according to GR/T1802.1, H is 160N, the number of times, the total number of times is 500 meters, and the test level is in accordance with G816132-2002:
5.4.10 Methyl acetate content test
Perform the provisions of (/,:). 5.4.11 pH value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11,HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate according to the external quality yellow core batch. If the rate of non-conforming products is within the range of 7 and below, the batch of products is qualified. If the rate of non-conforming products is above the range of 7, the batch of products is qualified.
6.1.2 Inner packaging mark is calculated, and no external error is allowed. 6.2 Inner quality
6.2.1 The inspection results will be taken from the adjacent test samples, and the qualified ones will be judged as qualified, and the unqualified ones will be judged as unqualified. 6.2.2 Calculate the dimensional change rate of all test samples and the result with acid. If the test results show that the batch of products are qualified, the unqualified ones will be determined as unqualified. If there is shrinkage and expansion test, the value of the calculated value (or the value selected by the test frequency) will be used as the test result. If the batch of products are qualified, the batch of products will be determined as qualified, and the unqualified ones will be determined as unqualified. 6.2.3 For formaldehyde content, for light color, for color flatness, for chromaticity, and for color flatness, the batch of products will be determined as qualified, and the unqualified ones will be determined as unqualified. : 6.2.4 The product performance of the product is not allowed to be released. 6.3 Re-inspection || tt || 6.3.1 The results of the inspection are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to the friend for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection time is the designated inspection quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations will be implemented, and the inspection will be based on it. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.2 Product packaging technology G.T4856 or cooperative implementation,8 Light fastness and perspiration test
According to GHT157S+B
5.4.9 Test
According to GR/T1802.1, H is 160N, the number of times, the number of times is 500 times, the level is G816132-2002:
5.4.10 Methyl acetate content test
According to (/,: Regulations. Special treatment products are tested for special treatments such as rate, speed, etc. 5.4.11 pH Value test
According to G/T7:?3 regulations
5.4.12 Fiber content test
Fz/17302:—2004
According to GH/1251C.GB/T251-.FZ/TUU57.1~1U57.11, HZ/T01C95 and other standards. 5.4.13 Color fastness rating
According to G325, G3251.
6 Judgment criteria
6.1 Appearance quality
6.1.1 Calculate the non-conforming product rate for the external quality inspection batch. The non-conforming product rate is within the range of 7.7, and the batch is qualified. If the non-conforming product rate is above the center, the batch is qualified.
6.1.2 The internal packaging mark is calculated. No external errors are allowed. 6.2 Internal quality
6.2.1 The test results are taken from the adjacent test samples. The qualified ones are judged as qualified, and the unqualified ones are judged as unqualified. 6.2.2 Calculate the size change rate of all the test samples and the technical level. If the shrinkage and expansion test results exist, the batch of products will be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.3 The aldehyde content of PET fiber shall be judged as qualified, and those that are unqualified will be judged as unqualified. 6.2.4 The product content shall be judged as qualified, and those that are unqualified will be judged as unqualified. The product with small capacity for taking performance is allowed.6.3 Re-inspection
6.3.1 The results of the test are calculated. Within the specified period of 4 hours, all the agreed objects can be as complete as possible: 6.3.2 When reporting to friends for inspection, it is hoped that all the quantities of mutual inspection are guaranteed. 6.3.3 When re-inspecting, the inspection efficiency disk is the designated inspection efficiency quantity. The refrigeration station will follow the standard of this clause (1.6.2 The current regulations shall be implemented, and the inspection shall prevail. 7 Product instructions for use, packaging, transportation and storage 7.1 Instructions for use follow R296. Original operation. 7.
Tip: This standard content only shows part of the intercepted content of the complete standard. If you need the complete standard, please go to the top to download the complete standard document for free.