title>General requirements and test methods of paper and printing qualities for primary and secondary school textbooks - GB/T 18359-2001 - Chinese standardNet - bzxz.net
Home > GB > General requirements and test methods of paper and printing qualities for primary and secondary school textbooks
General requirements and test methods of paper and printing qualities for primary and secondary school textbooks

Basic Information

Standard ID: GB/T 18359-2001

Standard Name:General requirements and test methods of paper and printing qualities for primary and secondary school textbooks

Chinese Name: 中小学教科书用纸、印制质量标准和检验方法

Standard category:National Standard (GB)

state:Abolished

Date of Release2001-06-07

Date of Implementation:2001-06-07

Date of Expiration:2009-12-01

standard classification number

Standard ICS number:Imaging Technology>>Printing Technology>>37.100.01 Printing Technology General

Standard Classification Number:General>>Economy, Culture>>A17 Printing Technology

associated standards

alternative situation:Replaced by GB/T 18359-2009

Publication information

publishing house:China Standards Press

other information

Release date:2001-06-07

Review date:2004-10-14

Drafting unit:China Institute of Printing Science and Technology

Focal point unit:National Printing Standardization Technical Committee

Publishing department:General Administration of Quality Supervision, Inspection and Quarantine

competent authority:State Press and Publication Administration

Introduction to standards:

This standard specifies the paper used for primary and secondary school textbooks, printing quality requirements and inspection methods. This standard applies to various textbooks used in ordinary primary and secondary schools. Teaching auxiliary books used by primary and secondary school students can refer to this standard. GB/T 18359-2001 Paper used for primary and secondary school textbooks, printing quality standards and inspection methods GB/T18359-2001 Standard download decompression password: www.bzxz.net
This standard specifies the paper used for primary and secondary school textbooks, printing quality requirements and inspection methods. This standard applies to various textbooks used in ordinary primary and secondary schools. Teaching auxiliary books used by primary and secondary school students can refer to this standard.


Some standard content:

GH/T18359-2001
The wood standard is based on the international and domestic relevant standards, and is revised according to its own teaching paper, printing quality requirements and inspection methods in combination with the current actual situation of China.
This standard is proposed by the General Administration of Press and Publication of the People's Republic of China and is under the jurisdiction of the National Information and Publication Standardization Technical Committee Publication Technical Committee. The drafting units of this standard are: China Printing Technology Research Institute, China Papermaking Research Institute, and People's Publishing House. The main drafters of this standard are Ji Jiayang, Chen Ci, Sha Xiaoqing, Gan Aizhen, and others.
National Standard of the People's Republic of China
Primary and secondary school textbook paper, printing quality standards and inspection methods
General requirements and standards of primary and secondary school textbooks
This standard defines ten requirements and inspection methods for primary school textbook paper, printing quality, GB/T 18359.2001
This standard is based on various textbooks used in primary and secondary schools. This standard can be used as a reference for supplementary teaching materials and other textbooks for primary and secondary school students.
? Reference Standards
The following references contain clauses that are cited in the references and become the clauses of this standard: When the standard is issued, the versions shown are valid: All standards will be revised, and the parties using this standard should explore the possibility of using the following references as the latest version. 3/T4-:1989 Paper and paperboard sample taking (9S01861585) G/4.:1.1-19H9 Paper and needle tax size and deflection determination method 3/1451.21989 Paper and paper version determination or attached CVTS) G:1976) C3/T461.3-1989
(F/453198! Low and paperboard strength and elasticity determination method (constant rate gain method) (cqVI9924-1.1983) GB/T 45G-1989
GBT4571989
GB/T 46C—118
H/T462—1989
Method for determination of smoothness of paper grade board (E562%:994 Method for determination of paper folding degree (EG15) M20197%) Determination of sizing degree of both board and paperboard (Cui Shu Bei Xian Ran) Determination of moisture content of paper and paperboard (Extension method 50287:17GBT1511-1986
GB/T5131966
Method for determination of dust content of paper and paper
Determination of dust content of paper (+182471:97)
GI5/T -545.1—1589
GB/T 2579. 15.-
Shu, board and grade pulp water extraction from acid skin or magnetic determination method for paper and paperboard printing strength determination by electric meter and electric method (537331980) GT/T 2679.16-1997
Buy and paper and paper printing surface strength determination (random or detailed accelerated method e91503782:1980) GB/7974188? Paperboard degree determination (micro-radio/multiplication method 2e4[S) 2270:1977) GT12141S91
Paper and paper speed determination (machine speed value determination> (e9V1S1S21-2.19R5) GB/985-1S5 Printing technical terminology
0/T10739-1989 Pulp. Paper and paperboard sample processing test standard atmosphere (m5O18% 1954) (B1731.20 Printing technology network daily adjustment color separation film, sample and printed product processing control second pre-separation
Printing eq15012617-2:1996)
GB/T 1X35X—2U31
General standard for the size and size of primary and secondary school textbooks Y73—1999 Specification and specification conditions General Administration of Quality Supervision, Inspection and Quarantine of the People's Republic of China 2001-06-07 Approval TTKAONKA
2001-06-07 Implementation
GB/T1A359—2001
CYT3-10 Quality requirements and inspection methods for planographic printed materials Y13—19 Quality requirements and inspection methods for printed books CY/Jiang2R1999 Quality requirements and inspection methods for binding—paperback YT29-1999 Quality requirements and inspection methods for binding 3 categories
Material and materials for single-color printing. 4.1 Paper requirements · Binding ... R/m
Resistance to megawatt
N·m/g
50 g/m
-to ghiu
no retreat,
positive three,
stop area in difference,%
average report weaving batch average
super teaching, m
car press, area
b.: - 2. u
60 - 3. (
74. 3-~$5. 3
10mr overpressure
7. U AU,
cultivation standard art song
*.? mm--fi.5 mm
of "calling more
.3. uut, sum.
's air volume will be T
,5 u dust
printing steel surface strength (positive layer positive average)./.
rate of water,
GA/T18359
table 1r complete 1
no
4. n~-g. f
4.3 the width deviation of the material should not exceed two * mm, the vertical deviation is 83mm=5vmm: the flat paper size deviation should not exceed +31 mm.
2.1.4 the sheet should not have the phenomenon of penetrating and falling powder on the sheet, the bottom of the sheet should be flat, the red single organization should be, the color should be consistent, and each sheet should not have obvious differences. 4.1.5 The brightness (width) of the same batch of paper is not increased. 4.1.6 The paper shall not be classified into external paper that affects the printing type, such as flat, folded, sensitive, and various stripes, spots, light-avoiding spots, eye spots, etc. The flat-grade paper shall not have paper pieces, broken sheets, damaged, burnt, etc. 4.1.7 The number of heads per roll shall not exceed 10. 4.1.8 The paper defects found during rewinding, such as obvious folds, wrinkles, streaks, spots, holes, etc., shall not exceed 10. Table 2 Color separation film requirements Color separation film composition meets:
) uniform density 3.5C;
b! Film base efficiency u.13
:) The selected part of the dot area is attached with a plan of% 0.1Ud) The number of dots (dot frequency: monochrome image is 4u line/ct--48 line/cm (0\ load/in~_21 line/im) color image is 1B line/en1~7u line/em!: 2U line/in~=75 line/in) science, dot high breakage:
color separation film quality reduction, element production trace:
) color separation diagonal courtyard registration is full of center difference, 4.3 printing requirements
4.3.1 American negative printing tape respect textbook
monochrome textbook printing should comply with food
) 1 example with color direction, printing element standard printing field abuse value, 9.91.6! 1) The text is clear, without shadows, missing lines, or blurred characters; 2) The image is clearly layered, the text in the figure is correct, and the position is accurate; 3) The table is clear, without creases or dirt; 4.3.2 The printing of color science textbooks should comply with GB/T18359-2001; 8) The solid color measurement should meet the requirements of Table 2. Table 2 Solid color measurement values ​​English (r) Black (E) The dot area reproduction range is ~3, and the text is clear and without ghosting.No obvious missing strokes, blurred characters, or bad printing; printing
c ~ - ns
1.ro--: 56
) The image is clearly layered, and the dot slips and the scanning reverse value = (:D should be combined with Table 3: Table 5 offset printing K estimation
focus (care)
e) overprinting and sending the ticket center.2mm!
Offset printing
c. 3) -cu
Remaining color to be printed, naturally, the same batch of products with the same color printing field allowable error should meet the requirements of Table 4 Table 4 Same batch of products with the same color printing density allowable error blue
Magenta (M)
Name) The layout is clean, no brightest fold wave stove reading, 4.4 Binding
Books and books can be bound as follows:
) Three folds and more than three folds, forget to remove air from the delivery port. Nine
Sheets / m\ and below paper maximum fold: 60/m~80/m paper maximum fold:! The card is flat and even, without wrinkles, dead folds, corners, warps, sets and speed. The code and order of the card are correct, with the midpoint as the correct one. The code control setting of the connection is allowed to be 0.00, and the error of the whole book code position is allowed. 1.00um: the picture connection is allowed to be 1.00um. The folding edge of the glue binding book is correct. The end is transparent, and the folding line is in the process of folding. 4.4.2 Card core binding
4.4.2.1 The requirements for book core glue binding are as follows:
1! The number of glue bindings should be combined with the relevant quality requirements: 1) Driving rate: 23mm-~3.0mm for three-fold book and 2.5mm-3.0mm for west-fold book to ensure that the adhesive can be lifted to the book, and there will be no loose, unstuck and back-folding phenomena. It is skewed (the top and bottom should be 31.0mm-134
1) and the thickness should be pressed, u.6 mm~.1.2:
4.4.2-2 The requirements for the flat binding of the book core wire are as follows: GD/T18359
The binding is 174 places above and below the outer core, and the error is allowed to be b.Umm. The distance between the book and the book is: the thickness of the book core is 1,3.0mm--6.mm, and the m is 4.0m~7.0mmh! Light saw, through binding, or binding: the binding is flat and firm. ! The root tape quality and book core thickness should be fixed with a smooth rust-free iron wire with a diameter of 0.5Cmm~C.75mra: 4.4.3 Opposite floor film, glazing
Cover and the title should be glazed
) The film is firmly bonded, the surface is flat and not blurred, and there is no reverse mark. The degree of treatment is good, without wrinkles, pools, powder marks and core film. The upper scale is small and accurate, without film, no obvious grid, bulging mouth 4.0mm.) The lower degree of light is suitable, and there is no large sticky surface or missing or stretching phenomenon. 1) After the film is released for 10h~h, the quality of the title will not change:) On the cover, there are no marks or traces.
444、≤Village surface
4.4.4.1 Requirements for adhesive book packaging and packaging: The width of the cover of the machine adhesive station is 3.U-7.m
b) The adhesive seal should be straight and flat
It is the three-dimensional section of the back plate after the type, without adhesive seal, large fold negative. ) The viscosity of the system should be appropriate, and the adhesive rate should be appropriate, without adhesive: 4.4..2 Requirements for wire sealing;
) According to the order of the core and cover paper, the correct month and the type of brake, the degree and use of the plate, with the book back fire push, case several.9: No obvious solution, the book cover length, half of the package, the same batch of books below 3.Vm. 1) Through the back, the book fee is half the whole. Fire pressure and fixed negative, etc. )State density is more than 2UR/, the glue edge should be indented, the book will be indented and the glue edge indentation difference is 1.Umm.
44.5 End Martin binding
and the binding should meet the following requirements:
:) The front post should be generally, and the quick alignment
6) The position of the book is limited to the upper and lower cores. The allowable error is 3.0mm: no, no order, double seal, flat production, flat style, semi-solid, evenly folded, and the book is not skewed.3tn
4.4.6 The quality of the finished product
textbooks should meet the following requirements: The book core should be straight, smooth, without protection, folding, discoloration, damage, and the glue edge meets the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first test.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logo. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKau
The remaining color is waiting for a sample to be printed, naturally, the same batch of products with the same color printing field tolerance error should meet the requirements of Table 4 Table 4 The same batch of products with the same color printing field tolerance error blue
Magenta (M)
Name) The layout is clean, no brightest fold wave stove reading, 4.4 Binding
Books and books can be bound as follows:
) Three folds and more than three folds, forget to remove air from the delivery port. Nine
Sheets/m\ and below The maximum fold of paper: 60/m~80/m The maximum fold of paper:! The card is flat and even, without wrinkles, dead folds, corners, warps, sets and speed. The code and order of the card are correct, with the midpoint as the correct one. The code control setting of the connection is allowed to be 0.00, and the error of the whole book code position is allowed. 1.00um: the picture connection is allowed to be 1.00um. The folding edge of the glue binding book is correct. The end is transparent, and the folding line is in the process of folding. 4.4.2 Card core binding
4.4.2.1 The requirements for book core glue binding are as follows:
1! The number of glue bindings should be combined with the relevant quality requirements: 1) Driving rate: 23mm-~3.0mm for three-fold book and 2.5mm-3.0mm for west-fold book to ensure that the adhesive can be lifted to the book, and there will be no loose, unstuck and back-folding phenomena. It is skewed (the top and bottom should be 31.0mm-134
1) and the thickness should be pressed, u.6 mm~.1.2:
4.4.2-2 The requirements for the flat binding of the book core wire are as follows: GD/T18359
The binding is 174 places above and below the outer core, and the error is allowed to be b.Umm. The distance between the book and the book is: the thickness of the book core is 1,3.0mm--6.mm, and the m is 4.0m~7.0mmh! Light saw, through binding, or binding: the binding is flat and firm. ! The root tape quality and book core thickness should be fixed with a smooth rust-free iron wire with a diameter of 0.5Cmm~C.75mra: 4.4.3 Opposite floor film, glazing
Cover and the title should be glazed
) The film is firmly bonded, the surface is flat and not blurred, and there is no reverse mark. The degree of treatment is good, without wrinkles, pools, powder marks and core film. The upper scale is small and accurate, without film, no obvious grid, bulging mouth 4.0mm.) The lower degree of light is suitable, and there is no large sticky surface or missing or stretching phenomenon. 1) After the film is released for 10h~h, the quality of the title will not change:) On the cover, there are no marks or traces.
444、≤Village surface
4.4.4.1 Requirements for adhesive book packaging and packaging: The width of the cover of the machine adhesive station is 3.U-7.m
b) The adhesive seal should be straight and flat
It is the three-dimensional section of the back plate after the type, without adhesive seal, large fold negative. ) The viscosity of the system should be appropriate, and the adhesive rate should be appropriate, without adhesive: 4.4..2 Requirements for wire sealing;
) According to the order of the core and cover paper, the correct month and the type of brake, the degree and use of the plate, with the book back fire push, case several.9: No obvious solution, the book cover length, half of the package, the same batch of books below 3.Vm. 1) Through the back, the book fee is half the whole. Fire pressure and fixed negative, etc. )State density is more than 2UR/, the glue edge should be indented, the book will be indented and the glue edge indentation difference is 1.Umm.
44.5 End Martin binding
and the binding should meet the following requirements:
:) The front post should be generally, and the quick alignment
6) The position of the book is limited to the upper and lower cores. The allowable error is 3.0mm: no, no order, double seal, flat production, flat style, semi-solid, evenly folded, and the book is not skewed.3tn
4.4.6 The quality of the finished product
textbooks should meet the following requirements: The book core should be straight, smooth, without protection, folding, discoloration, damage, and the glue edge meets the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first measurement.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logos. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKau
The remaining color is waiting for a sample to be printed, naturally, the same batch of products with the same color printing field tolerance error should meet the requirements of Table 4 Table 4 The same batch of products with the same color printing field tolerance error blue
Magenta (M)
Name) The layout is clean, no brightest fold wave stove reading, 4.4 Binding
Books and books can be bound as follows:
) Three folds and more than three folds, forget to remove air from the delivery port. Nine
Sheets/m\ and below The maximum fold of paper: 60/m~80/m The maximum fold of paper:! The card is flat and even, without wrinkles, dead folds, corners, warps, sets and speed. The code and order of the card are correct, with the midpoint as the correct one. The code control setting of the connection is allowed to be 0.00, and the error of the whole book code position is allowed. 1.00um: the picture connection is allowed to be 1.00um. The folding edge of the glue binding book is correct. The end is transparent, and the folding line is in the process of folding. 4.4.2 Card core binding
4.4.2.1 The requirements for book core glue binding are as follows:
1! The number of glue bindings should be combined with the relevant quality requirements: 1) Driving rate: 23mm-~3.0mm for three-fold book and 2.5mm-3.0mm for west-fold book to ensure that the adhesive can be lifted to the book, and there will be no loose, unstuck and back-folding phenomena. It is skewed (the top and bottom should be 31.0mm-134
1) and the thickness should be pressed, u.6 mm~.1.2:
4.4.2-2 The requirements for the flat binding of the book core wire are as follows: GD/T18359
The binding is 174 places above and below the outer core, and the error is allowed to be b.Umm. The distance between the book and the book is: the thickness of the book core is 1,3.0mm--6.mm, and the m is 4.0m~7.0mmh! Light saw, through binding, or binding: the binding is flat and firm. ! The root tape quality and book core thickness should be fixed with a smooth rust-free iron wire with a diameter of 0.5Cmm~C.75mra: 4.4.3 Opposite floor film, glazing
Cover and the title should be glazed
) The film is firmly bonded, the surface is flat and not blurred, and there is no reverse mark. The degree of treatment is good, without wrinkles, pools, powder marks and core film. The upper scale is small and accurate, without film, no obvious grid, bulging mouth 4.0mm.) The lower degree of light is suitable, and there is no large sticky surface or missing or stretching phenomenon. 1) After the film is released for 10h~h, the quality of the title will not change:) On the cover, there are no marks or traces.
444、≤Village surface
4.4.4.1 Requirements for adhesive book packaging and packaging: The width of the cover of the machine adhesive station is 3.U-7.m
b) The adhesive seal should be straight and flat
It is the three-dimensional section of the back plate after the type, without adhesive seal, large fold negative. ) The viscosity of the system should be appropriate, and the adhesive rate should be appropriate, without adhesive: 4.4..2 Requirements for wire sealing;
) According to the order of the core and cover paper, the correct month and the type of brake, the degree and use of the plate, with the book back fire push, case several.9: No obvious solution, the book cover length, half of the package, the same batch of books below 3.Vm. 1) Through the back, the book fee is half the whole. Fire pressure and fixed negative, etc. )State density is more than 2UR/, the glue edge should be indented, the book will be indented and the glue edge indentation difference is 1.Umm.
44.5 End Martin binding
and the binding should meet the following requirements:
:) The front post should be generally, and the quick alignment
6) The position of the book is limited to the upper and lower cores. The allowable error is 3.0mm: no, no order, double seal, flat production, flat style, semi-solid, evenly folded, and the book is not skewed.3tn
4.4.6 The quality of the finished product
textbooks should meet the following requirements: The book core should be straight, smooth, without protection, folding, discoloration, damage, and the glue edge meets the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first test.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logo. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKa5mm-3.mm. to ensure that the adhesive can penetrate the book, and there will be no loose, peeling and back folding. It is skewed (the top and bottom should be 31.0mm134
1) and the thickness should be pressed, u.6 mm~.1.2:
4.4.2-2 The requirements for the flat binding of the book core wire are as follows: GD/T18359
The binding is 174 places above and below the outer core, and the error is allowed. Umm. The distance between the book and the book: the book core thickness is 1,3.0mm--6.mm and the m is 4.0m~7.0mmh! Light saw, through binding, or binding: the binding is flat and firm. ! The root tape quality and book core thickness should be fixed with a smooth rust-free iron wire with a diameter of 0.5Cmm~C.75mra: 4.4.3 Opposite floor film, glazing
Cover and the title should be glazedbzxz.net
) The film is firmly bonded, the surface is flat and not blurred, and there is no reverse mark. The degree of treatment is good, without wrinkles, pools, powder marks and core film. The upper scale is small and accurate, without film, no obvious grid, bulging mouth 4.0mm.) The lower degree of light is suitable, and there is no large sticky surface or missing or stretching phenomenon. 1) After the film is released for 10h~h, the quality of the title will not change:) On the cover, there are no marks or traces.
444、≤Village surface
4.4.4.1 Requirements for adhesive book packaging and packaging: The width of the cover of the machine adhesive station is 3.U-7.m
b) The adhesive seal should be straight and flat
It is the three-dimensional section of the back plate after the type, without adhesive seal, large fold negative. ) The viscosity of the system should be appropriate, and the adhesive rate should be appropriate, without adhesive: 4.4..2 Requirements for wire sealing;
) According to the order of the core and cover paper, the correct month and the type of brake, the degree and use of the plate, with the book back fire push, case several.9: No obvious solution, the book cover length, half of the package, the same batch of books below 3.Vm. 1) Through the back, the book fee is half the whole. Fire pressure and fixed negative, etc. )State density is more than 2UR/, the glue edge should be indented, the book will be indented and the glue edge indentation difference is 1.Umm.
44.5 End Martin binding
and the binding should meet the following requirements:
:) The front post should be generally, and the quick alignment
6) The position of the book is limited to the upper and lower cores. The allowable error is 3.0mm: no, no order, double seal, flat production, flat style, semi-solid, evenly folded, and the book is not skewed.3tn
4.4.6 The quality of the finished product
textbooks should meet the following requirements: The book core should be straight, smooth, without protection, folding, discoloration, damage, and the glue edge meets the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first measurement.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logos. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKa5mm-3.mm. to ensure that the adhesive can penetrate the book, and there will be no loose, peeling and back folding. It is skewed (the top and bottom should be 31.0mm134
1) and the thickness should be pressed, u.6 mm~.1.2:
4.4.2-2 The requirements for the flat binding of the book core wire are as follows: GD/T18359
The binding is 174 places above and below the outer core, and the error is allowed. Umm. The distance between the book and the book: the book core thickness is 1,3.0mm--6.mm and the m is 4.0m~7.0mmh! Light saw, through binding, or binding: the binding is flat and firm. ! The root tape quality and book core thickness should be fixed with a smooth rust-free iron wire with a diameter of 0.5Cmm~C.75mra: 4.4.3 Opposite floor film, glazing
Cover and the title should be glazed
) The film is firmly bonded, the surface is flat and not blurred, and there is no reverse mark. The degree of treatment is good, without wrinkles, pools, powder marks and core film. The upper scale is small and accurate, without film, no obvious grid, bulging mouth 4.0mm.) The lower degree of light is suitable, and there is no large sticky surface or missing or stretching phenomenon. 1) After the film is released for 10h~h, the quality of the title will not change:) On the cover, there are no marks or traces.
444、≤Village surface
4.4.4.1 Requirements for adhesive book packaging and packaging: The width of the cover of the machine adhesive station is 3.U-7.m
b) The adhesive seal should be straight and flat
It is the three-dimensional section of the back plate after the type, without adhesive seal, large fold negative. ) The viscosity of the system should be appropriate, and the adhesive rate should be appropriate, without adhesive: 4.4..2 Requirements for wire sealing;
) According to the order of the core and cover paper, the correct month and the type of brake, the degree and use of the plate, with the book back fire push, case several.9: No obvious solution, the book cover length, half of the package, the same batch of books below 3.Vm. 1) Through the back, the book fee is half the whole. Fire pressure and fixed negative, etc. )State density is more than 2UR/, the glue edge should be indented, the book will be indented and the glue edge indentation difference is 1.Umm.
44.5 End Martin binding
and the binding should meet the following requirements:
:) The front post should be generally, and the quick alignment
6) The position of the book is limited to the upper and lower cores. The allowable error is 3.0mm: no, no order, double seal, flat production, flat style, semi-solid, evenly folded, and the book is not skewed.3tn
4.4.6 The quality of the finished product
textbooks should meet the following requirements: The book core should be straight, smooth, without protection, folding, discoloration, damage, and the glue edge meets the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first measurement.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logos. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKa5. The mounting and installation should comply with the following requirements: 1. The front post should be generally straight, 2. The back post should be aligned, 3.0mm is allowed at the upper and lower 1/1 of the core, and the error is limited to 3.0mm. There is no order, no double sealing, flat production, flat style, semi-solid, evenly folded, straightened online, no crooked sticking, etc. 4.4.6. The quality of finished textbooks should meet the following requirements: The book core should be straight, smooth, without any protection, folding, discoloration or damage, and the adhesive edge should meet the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first measurement.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logos. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKa5. The mounting and installation should comply with the following requirements: 1. The front post should be generally straight, 2. The back post should be aligned, 3.0mm is allowed at the upper and lower 1/1 of the core, and the error is limited to 3.0mm. There is no order, no double sealing, flat production, flat style, semi-solid, evenly folded, straightened online, no crooked sticking, etc. 4.4.6. The quality of finished textbooks should meet the following requirements: The book core should be straight, smooth, without any protection, folding, discoloration or damage, and the adhesive edge should meet the requirements. w1.uxm.
h finished product virtual surface size effect (H1835s provisions, size coupon 11., m. non-standard size required according to the contract requirements e product cutting enterprise material wet left 1nir
finished product or after cutting without strict knife can be too visible, especially serious sold. c: the back of the word half shift error based on the book center line, the back of the book thickness of 1 and below the finished book, the back of the book translation error mn Zhuo perfect greater than the finished product, the back of the book enjoy more than 20mm allowable error: notice The allowable error of the back text of the finished book with a thickness of more than 23mm and less than or equal to 30mm is 2.mm; the allowable error of the back text of the finished book with a back pressure of more than mm is smaller than the allowable error of the back text.rm
TTKAONKa
CB/I183552001
f) The folding edge of the sealed mouth is aligned with the front edge of the core, with a temperature difference of 1.0mm) The finished product has a smooth appearance and no indentation. 5 Inspection methods
5.1 Paper strength quality inspection
5.1.1 Sample collection and treatment shall be carried out in accordance with the provisions of GI3/T45 standard GB:TU739. 5.1.2 Paper size and tolerance inspection shall be carried out in accordance with the provisions of GT45_.1. 5.1.3 Quantitative inspection of sheets shall be carried out in accordance with the provisions of GT2i1. 5.1.4 Paper thickness inspection shall be carried out in accordance with the provisions of GB/1451.5. 5.1.5 Sheet width (mm) shall be carried out in accordance with the provisions of C/T7974. 5.1.6 Paper opacity inspection shall be carried out in accordance with the provisions of GB/1543. 5.1.7 Paper smoothness inspection shall be carried out in accordance with the provisions of GBT1543. 5.1.8 The expansion index test of paper shall be carried out in accordance with the provisions of GBT453 and G/12914. In case of any dispute, arbitration shall be carried out in accordance with G/12914. The expansion index test of paper shall be carried out in accordance with the provisions of GB/T60 and the "Paper Double Filter and Expansion Ratio" shall be implemented. 10
The dust test of paper shall be carried out in accordance with GB/T1541. 5.1.11
The folding endurance test of paper shall be carried out in accordance with GB457. The non-H test of paper shall be carried out in accordance with GB/T4545.】. 5.1.12
The moisture test of paper shall be carried out in accordance with GB/T452. 5.1.14 For the determination of most paper defects of paper, take the outer 10 layers of two sheets of paper, stop at the outermost 3 layers, and the remaining 5 layers as the test length, and make them into 5-2” pieces, select samples and For the defective film, calculate the white content ratio of the test column. 5.1.15 The surface test of several printed sheets shall be carried out in accordance with the provisions of GB/T257\.15 and G3/2679.16, and domestic low-viscosity waste oil shall be used. If there is any dispute, arbitration shall be carried out in accordance with CB/T2671: 5.2 Printing quality inspection
5.2.1 Inspection conditions
The printing quality inspection conditions shall meet the requirements of
The working environment shall be neutral, some clean:) The working environment temperature (23 above) is relatively wet (52) yuan:) Color prints must check the light source 5.2.2 Inspection instruments or tools
Printing quality inspection instruments or 1 as follows:
: Densitometer that meets the requirements and is in compliance with the inspection requirements: 6) 0--100 confidence magnifying glass:
c1015 times bandpass magnifying glass!
d) Measurement strips
e) For black base agents with no selection, careful reflection, and a reflection density of 1._0.29: 5.2.3 Inspection method
Printing quality inspection method
E) Single measurement method: || tt||h calculation method
r) measurement method,
d) comparison string:
center) expert identification method.
5.3 Packing quality inspection method
Packaging quality inspection method is as follows
) measurement method
b) first measurement.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printed and reported special packaging materials for reduced products, packaging: The packaging has the relevant standards and established drug logos. 6. 7 Delivery
It is not allowed to step on, press or drop from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 Storage
Open environment change, keep the degree of road appropriate, pay attention to point to prevent questions, prevent the emergency, oil break range, follow the fiber, prevent the sinking can not be single pressure TKAONKa3 Inspection method
Printing quality inspection method
e) Measurement method:
h Calculation method
r) Measurement method,
d) Comparison method:
center) Expert identification method.
5.3 Packing quantity inspection method
Packaging quality inspection method is as follows:
) Measurement method
b) First test.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printing special packaging materials for reduced products, packaging: The packaging has a drug logo that meets relevant standards and is established. 6. 7 Send static
Do not allow joint stepping, heavy pressure or throwing from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 save
open the environment to change, ensure the degree of road, pay attention to point prevention, prevention of emergency, oil cut range, follow the fiber, and prevent sinking. Do not press TKAONKa alone3 Inspection method
Printing quality inspection method
e) Measurement method:
h Calculation method
r) Measurement method,
d) Comparison method:
center) Expert identification method.
5.3 Packing quantity inspection method
Packaging quality inspection method is as follows:
) Measurement method
b) First test.
6 Packaging, transportation, storage
6.1 Packaging
GB/T18359
Printing special packaging materials for reduced products, packaging: The packaging has a drug logo that meets relevant standards and is established. 6. 7 Send static
Do not allow joint stepping, heavy pressure or throwing from a high place, pay attention to the state of rain, sun, sun, brain, 5.3 save
open the environment to change, ensure the degree of road, pay attention to point prevention, prevention of emergency, oil cut range, follow the fiber, and prevent sinking. Do not press TKAONKa alone
Tip: This standard content only shows part of the intercepted content of the complete standard. If you need the complete standard, please go to the top to download the complete standard document for free.